Glaze Defect Guide: find the cause, then test it.

Pick what you see on the fired piece. Tick what applies. The guide narrows the list to the likely causes and tells you which test tile will confirm each one. No photos needed.

Running · Crawling · Pinholing · Crazing

Paper-collage row of four test tiles showing running, crawling, pinholing and crazing glaze defects.
1. What went wrong?
2. Tick anything that applies
Application
Firing
Clay body
Glaze age

The list updates as you tick. Your choices stay on this device.

Likely causes, most relevant first

Choose a defect to see its causes.

Running

What it looks like: glaze has flowed down the wall, pooled at the foot or reached the shelf.

Likely causeTest to confirm
Coat too thickDip two tiles, one with a single dip and one with a double dip. Fire them side by side, standing at a steep angle.
Fired past the glaze's coneFire a tile with a witness cone next to it and check the cone after firing.
A naturally fluid glazeFire one tile at a steep angle with a catch dish underneath and see how far it moves at normal thickness.
Layered glazes melting togetherFire one tile with each glaze alone and one with both layered. Compare.
Glaze too close to the footGlaze the next test with the bottom edge left bare and compare.

Next step: Check your recipe in Run Risk Check


Crawling

What it looks like: the glaze has pulled back into beads or islands and left bare clay, often with a thick rolled edge.

Likely causeTest to confirm
Dust, oil or handling marks on the bisqueGlaze two tiles: one wiped clean with a damp sponge and dried, one as it was. Fire together.
Coat too thick, cracking as it driedLook at the unfired coat for cracks. Then fire a thin-coat tile beside a thick-coat tile.
Too much raw clay shrinking in the coatMix a small batch with part of the raw clay replaced by calcined clay. Fire it beside the original.
Poor adhesion of the coatAdd a small amount of gum or binder to a test batch and compare.
A stiff, high-surface-tension glaze (often matte)Test a batch with slightly more flux and see whether it flows out.

Next step: Check your recipe in Run Risk Check


Pinholing

What it looks like: tiny pin-sized holes in the surface, sometimes down to the clay. Pitting is similar, with slightly larger shallow craters.

Likely causeTest to confirm
Gas from the body or glaze escaping late, with no time to healFire a tile with a hold at peak temperature beside one without.
Incomplete burnout in the bisqueBisque a tile more slowly, or slightly hotter, then glaze and fire it beside a normal one.
Coat too thick, trapping bubblesFire a thin-coat tile beside a thick-coat tile.
Glaze underfired or too stiff to healFire a tile slightly hotter and compare.
Gassing materials (for example zinc oxide or rutile)Test a batch with less of that material, or a calcined version.

Tip: rubbing visible pinholes in the unfired coat can fill them before firing.

Next step: Check your recipe in Run Risk Check


Crazing

What it looks like: a network of fine cracks in the glaze. It can appear straight from the kiln or weeks later. On functional ware it matters because cracks can hold bacteria or let liquid seep in.

Likely causeTest to confirm
Glaze shrinks more than the clay body on cooling (expansion mismatch)Fire the same glaze on two different clay bodies and compare.
A new or changed clay bodyFire the glaze on a tile of your old body and the new body together.
High-expansion fluxes such as sodium and potassiumTest a batch with less soda or potash feldspar, or more silica, and compare.
Thick coat adding stressFire a thin-coat tile beside a thick-coat tile.
Fast coolingFire a tile with a slower cool. This can reduce crazing but does not fix the mismatch.

Note: some potters use crazing on purpose in crackle glazes. On pots for food and drink, treat it as a defect, and have finished ware lab-tested if food safety is in question.

Next step: Compare a lower-expansion swap in the Material Swap Helper · Check your recipe in Run Risk Check